1.What is the temperature range for electrolytic degreasing of cold-rolled coils?
The electrostatic degreasing process temperature for cold-rolled coils is typically controlled between 60℃ and 85℃, with a typical operating temperature of 80℃±5℃.
Conventional electrostatic degreasing of cold-rolled strip: 80℃±5℃
Cold-rolled strip cleaning for galvanized/aluminized zinc wire: 60-85℃
Cold-rolled sheet pre-annealing cleaning: 60-85℃
Some low-temperature degreasing agents: 20-40℃ (suitable for specific conditions)

2.Why is heating necessary for electrolytic degreasing? How does temperature affect the degreasing effect?
Accelerated Saponification: Oils react with alkali solutions at high temperatures to form soluble soap. For every 10℃ increase in temperature, the saponification rate increases by approximately 1-2 times.
Reduced Oil Viscosity: High temperatures significantly reduce the viscosity of oils such as rolling oil and leveling fluid, increasing their fluidity and making them easier to peel off from the strip surface and be washed away by air bubbles.
Enhanced Emulsification: Surfactants have stronger emulsifying capabilities at high temperatures, stably dispersing the peeled oil in the degreasing solution and preventing re-adhesion.
Improved Electrolysis Efficiency: At suitable temperatures, the electrolyte conductivity increases, resulting in more uniform and denser bubble formation and enhanced mechanical peeling.
However, higher temperatures are not always better-temperatures exceeding 90℃ can lead to excessive alkaline mist generation, worsening the operating environment, accelerating equipment corrosion, and potentially rendering some surfactants ineffective.

3.What quality problems can occur when the electrolytic degreasing temperature is too low (<60℃)?
Incomplete saponification and inadequate removal of residual oil result in an oil film remaining on the steel strip surface.
During subsequent annealing, the oil carbonizes, forming "oil spots" or causing surface color variations.
The electrolytic bubbles are large and uneven, leading to poor localized degreasing.

4.What quality problems can occur when the temperature is too high (>90℃)?
Increased alkali evaporation leads to large fluctuations in bath concentration and increased degreasing agent consumption.
A large amount of alkali mist is generated, which may be carried into subsequent cleaning stages with the strip steel, affecting rinsing effectiveness.
Some alloying elements (such as Si and Mn) may undergo selective corrosion in a high-temperature alkaline environment.
For sensitive materials such as high-strength steel and galvanized substrates, this may affect surface activity.
5.How to achieve precise control of electrolytic degreasing temperature during production?
External Heat Exchanger Heating: The degreasing liquid is circulated and heated via a heat exchanger, resulting in good temperature uniformity.
In-Tank Immersion Heater: Fast heating response, but attention must be paid to localized overheating.
Steam Heating: High thermal efficiency, suitable for large-scale continuous production lines.
Multiple thermocouples are installed at the inlet, middle, and outlet of the degreasing tank to monitor temperature distribution in real time.
Temperature difference within the control area <= ±2℃, ensuring uniform temperature across the strip width.
The PLC automatically adjusts the opening of the heating steam valve or the heater power based on the deviation between the measured temperature and the set value.
Speed-Sensitive Integration: Heating power is automatically increased when the belt speed increases to compensate for heat loss.